Intaglio printing plate electroplating process - Chrome plating: Production precautions!
Release Time:
Nov 01,2017
Production Precautions
(a) The Effect of Chromic Anhydride Concentration
The chromic anhydride concentration in general plating solutions varies between 190 and 250 g/L. As the concentration of chromic anhydride increases, the conductivity of the plating solution improves, and the covering ability also increases, while the cathodic current efficiency decreases. After adding certain additives, the concentration effect becomes secondary. Typically, the concentration of the plating solution can be determined by the specific gravity method, and the relationship between chromic anhydride content and Baume degree is shown in the figure.

Xianmai Tu has newly developed an automatic chromic anhydride replenishment device that addresses the difficulties of chromic anhydride replenishment and concentration control. Its quality and performance have been validated by the market and received high recognition and praise from users. The functional advantages are as follows:
1. Mechanical stirring (time controllable) to avoid impurities entering the solution;
2. Hourly replenishment control managed by the plating tank PLC to avoid inaccurate ampere-hours;
3. Liquid level display and alarm replenishment (quantitative replenishment is convenient and intuitive);
4. Convenient replenishment of chromic anhydride (six barrels can be replenished in a few minutes);
5. Distribution and replenishment tanks, with valves closed during replenishment to avoid uneven solution;
6. The dosing pump is powerful, accurate, and durable, capable of remote replenishment, with a one-year warranty;
7. The tank design is precise, with a 10 cm liquid level for each barrel of chromic anhydride, facilitating the calculation of chromic anhydride and pure water replenishment amounts.
Automatic chromic solution replenishment device ↓↓
(b) The Effect of Sulfuric Acid Concentration
In the chromium plating process, sulfuric acid acts as a catalyst, dissolving the basic chromate gel film, allowing chromium to precipitate smoothly. The concentration of sulfuric acid has a significant impact on the quality of the chromium layer, and the important factor is the ratio of chromic anhydride to sulfuric acid, rather than the absolute content of sulfuric acid. When CrO3/SO42-=100, the current efficiency is highest; when CrO3/SO42-=95 (i.e., H2SO4 content is slightly high), the smoothness and density of the chromium layer are good, but the current efficiency and covering ability decrease, and the edges of the plating drum may appear white; when CrO3/SO42- >100 (i.e., H2SO4slightly low), the covering ability is better, but the smoothness of the chromium layer decreases, resulting in mottling and roughness. The effect of sulfuric acid on the cathodic reaction is shown in the figure.

If the sulfuric acid content in the plating solution is too high, barium carbonate (BaCO3) can be used to precipitate excess sulfuric acid, with the reaction as follows: H2SO4 + BaCO3 →BaSO4↓ + CO2↑ + H2O
2One gram of BaCO3 can precipitate one gram of H2SO4.
(c) The Effect of Trivalent Chromium
In addition to the necessity of containing chromic anhydride and sulfuric acid, the plating solution should also contain a certain amount of trivalent chromium. The plating solution must be electrically treated to generate a certain amount of trivalent chromium. Generally, the cathode in plating companies uses carbon brushes, while the anode uses lead-antimony alloy bars, and some use titanium-platinum alloy. It is recommended to use the German sintered titanium-based platinum-coated anode from Maituo Company, whichadopts THE-process sintering technology,is a high-end insoluble anode with a uniform coating, low internal stress, no voids, good toughness, and excellent bonding strength,achieving the best quality performance currently available internationally,and is used by the vast majority of high-end customers.


The German sintered anode has excellent electrochemical performance, low oxygen evolution potential, which helps reduce production energy consumption and lower anode operating temperature; excellent oxidation capability,ensuring the balance of trivalent chromium content in the plating solution and the stability of the solution composition;due to its special surface structure, it ensures that the volume of bubbles generated by the anode during production is relatively large, resulting in less carryover of the plating solution, reducing the consumption of chromic anhydride and other raw materials;;Lifetime Advantages ↓
1.37 timesthat of domestic anodes (the area coefficient of domestic anodes is 1.4, while that of the German sintered anode is1.92);The platinum coating of the German sintered anode
can be recycled and reused,and can be reused at leasttwice as long as the titanium substrate is intact.The German sintered anode has undergone the most scientifically rigorous glass bead blasting bonding strength tests, as shown in the figure:.
Each set of anodes comes with a complete inspection report, alleviating customers' concerns.

During production, the area ratio of the anode to the cathode is controlled at 2:1 or 3:2 to maintain the stability of trivalent chromium. If the trivalent chromium content is low, a large cathode and small anode should be used for electrolysis; if the trivalent chromium content is high, the anode area should be increased, and the cathode area should be reduced for electrolysis. At a temperature of 50-60°C, a current density of 5-10 A/dm
生产中,阳极与阴极面积比控制在2∶1或3∶2,可以保持三价铬的稳定。三价铬含量低,采用大阴极小阳极电解;三价铬含量高,则应增大阳极面积,减少阴极面积进行电解。在温度为50~60℃时,用电流密度为5~10A/dm2The current is powered for 2 to 4 hours until the trivalent chromium reaches the process requirements. In medium concentration plating solutions, some companies specify the trivalent chromium content as 1 to 5 g/L, while others specify it as 2 to 5 g/L. Practice shows that low trivalent chromium content results in slow chromium deposition speed, soft plating, and poor coverage ability; high trivalent chromium content leads to dull and rough plating, poor brightness, and a smaller range of bright current density. When the trivalent chromium content is too high, use a fine iron rod as the cathode, making the anode area about 10 to 30 times that of the cathode, with an anode current density of 1.5 to 2 A/dm.2until the trivalent chromium content is reduced to the specified range.
(d) Two methods for generating trivalent chromium
① Electrolytic treatment method: At a temperature of 50 to 60℃, use a small current (7 to 10 A/dm2) to install a waste plate roller for 30 hours to generate trivalent chromium ions.
② Chemical treatment method: Some companies add an appropriate amount of formaldehyde (analytical grade, 3000 g) to a 1000L main tank at a temperature of 50 to 60℃ and circulate for half an hour; some companies add an appropriate amount of hydrogen peroxide (1000 to 1500 g) to the 1000L main tank; generally, 1 gram of alcohol can generate 1.8 grams of trivalent chromium.
Leave Messags.
Any inquiries? questions? We’re here to help. Send us a message and we’ll be in touch.