Intaglio industry: Effective measures to prevent poor adhesion between the copper plating layer and the nickel plating layer!
Release Time:
Aug 22,2015
1. Fault phenomenon:
Poor adhesion of copper-nickel layer
Poor adhesion of copper-nickel layer
2. Fault analysis:
The adhesion between the nickel layer and the copper layer is poor. On one hand, this is due to the nickel layer being passivated before copper plating. On the other hand, it is caused by an imbalance in the proportion of additives in the copper plating bath or poor performance of the additives, leading to a large amount of decomposition products during use, which adversely affects the adhesion between the nickel and copper layers. Generally, in the first case, the nickel-plated roller will not be rinsed after nickel plating, and the crystals on the surface will evenly cover the surface, acting to isolate oxygen in the air and protect the nickel layer from oxidation. The grinding before copper plating further activates the nickel layer due to the presence of nickel chloride. Therefore, the situations encountered in production are mostly of the second type.
3. Rectification measures:
1. After nickel plating the roller, apply power within 10 seconds of entering the copper plating bath to prevent the nickel layer from becoming too thin and causing a replacement reaction between the iron substrate and copper ions. This also prevents the nickel layer from adsorbing the characteristics of the additives in the copper bath, affecting adhesion.
2. The small current ratio after the roller enters the copper plating bath should exceed 0.3 times. If there is a phenomenon of blackening at small currents, the small current ratio should be further increased.
3. Appropriately reduce the usage of additive 2# and supplement with additive 1# in moderation to suppress the side effects of additive 2#.
4. The copper plating solution should be regularly treated with activated carbon powder, with a cycle not exceeding one year.
5. Cleaning process before nickel plating: Sulfuric acid spray rust removal ------ rinsing ------ alkaline cleaning agent grinding and degreasing ------- pure water spray (not too long) ------- entering the copper bath. The goal is to leave a trace of alkaline solution on the surface of the roller after cleaning, with a pH value greater than 7, so that the roller will not rust for a relatively long time. This avoids the situation where the roller rusts before entering the nickel plating bath due to prolonged operation of the automatic line, which not only affects the quality of nickel plating but also contaminates the nickel plating solution.
6. Replace with a brand of additives with better overall performance, such as the acid copper specifically for gravure electroplating from Changjin Company.Electroplating additivesKY-Z, KY-GP series, all belong to leading technologyCopper plating additivesbrands that can effectively solve this problem.