Corrosion inside the gravure chrome layer - chrome peeling, experience sharing on problem solving


Release Time:

Jan 03,2017

The plate roller shows corrosion within the chrome layer after printing - a failure phenomenon of chrome shedding:

1. The area of chrome shedding on the plate roller is approximately 0.5*1-3 mm.

2. It appears in a spotty or flaky distribution on the plate surface, without regularity.

3. The occurrence probability is about 0.5%.

4. The diameter of the plate rollers is concentrated in the range of 130-180 mm, and large diameter rollers almost never exhibit similar failures.

Failure analysis:

1. There are always macro cracks at the places where chrome shedding occurs, and the underlying copper layer is blackish-brown, indicating corrosion.

2. It is suspected that the hardness brittleness of the chrome layer is too high, causing macro cracks during the use of the plate roller, leading to corrosion of the underlying copper, formation of oxides, and resulting in chrome shedding.

3. Many of the customer's plate rollers are reused multiple times, with very thin walls and low strength, leading to significant deformation during use, which requires high toughness of the coating. Once the coating is too brittle, it easily causes macro cracks in the chrome layer.

4. Image:

Rectification measures:

Improper electroplating process, in pursuit of high hardness and deposition speed, leads to high brittleness of the chrome layer, causing macro cracks after use. These cracks are penetrating, allowing the copper layer to come into contact with moist air, resulting in oxidation and chrome shedding. The following suggestions are made:

1. Chromic anhydridecontent should be at the upper limit, recommended at 260-280g/L. High concentration processes help improve the brightness and density of the coating, enhancing its toughness.

2. Adjust the customer's acid ratio to within the range of 100:1.15-1.2; too little sulfuric acid will increase the hardness of the coating and also increase brittleness.

3. The trivalent chromium should not exceed 4.5g/L; 4. The rotation speed should not be less than 0.5m/S;

5. Additive performance defects, while increasing hardness and deposition speed, also cause excessive brittleness of the coating.Pulse expansionGerman imported hard chrome plating process VOP-Cr873Micro-cracks are excellent, more than similar products, effectively enhancing the corrosion resistance of the chrome layer, as shown in the image:

6. The electroplating process temperature is too low, and excessive current density will also increase the brittleness of the coating.

7. Appropriately increasing the thickness of the roller material helps improve the rigidity of the plate roller, and the resistance to deformation will also increase, helping to reduce the probability of macro crack formation and decrease chrome shedding failures.